Summary for Test 2020-10-12-37-2

Test performed: ASTM D412-06a-re13

Project Information

Project IdentifiersProject ID: 88888
DEA: SMTL-STOCK
EFIS: SMTL-STOCK
DIST-CO-RTE-PM59---
Award DateNot set
Closeout DateNot set
Work DescriptionSpecial project for SMTL stock material. Object Code: 1025. J2 DEA: 912680.
Location DescriptionNot set
QA Service LevelNOT VERIFIED

Sample Information

Sample Taken Date10/12/2020 Sample Unique Key37
Will the laboratory/organization for which you are a member perform testing on this material sample?Yes Date that the sample was received by the laboratory/organization performing the testing10/16/2020
Sample typeQuality Assurance A brief description of the sampleBearing Pad
The quantity of what the sample constitutes1 From where was the sample collectedManufacturer
First name of sampler or witnessed byBrad Last name of sampler or witnessed byStreeter
Title of sampler Telephone number of sampler
Laboratory sample identification Linked DIME Sample ID
The fabricator/manufacturer/facility nameScougal Rubber Transportation Laboratory (TL) Number
Inspector Lot Number from the Transportation Laboratory (TL) Form Structure unique identifier
Structure name

Material Information

Material TypeSMTL TM1 - Elastomeric Bearing Pad Mfg. Lot Number(s)1616359
Material/Compound/Elastomer IDna Samples Representing1
Description (size).25"x8"x12" Comments
Description (Number of Shims)na Type of Bearing PadPlain
Description (Thickness of Shims)NA Manufacturer(s)Scougal Rubber
Batch Numberna

Test Details

DIME Sample ID: 2020-10-12-37
DIME Test ID: 2020-10-12-37-2
Testing Lab: CT HQ - Sacramento Structural Materials Testing Laboratory
Test Method: ASTM D412-06a-re13: Standard Test Methods for Vulcanized Rubber and Thermoplastic Elastomers-Tension
Test Release Date: 2020-10-20

Test Results


Number of specimens tested: 3
Unit of the Ultimate Tensile Values: lbf per sqr in
Input Type: Calculated
Tester's full name: spaine
Date of test: 10/19/2020
UTM: 2kip
Humidity: 50.00 %
Temperature: 72 F
Sample 1 Median Thickness: 0.074
Sample 1 Thickness all Within 0.003 inch?: Yes
Sample 1 Ultimate Tensile: 2487.33 lbf/in^2
Sample 1 Elongation (350% Min): Pass
Sample 2 Median Thickness: 0.074
Sample 2 Thickness all Within 0.003 inch?: Yes
Sample 2 Ultimate Tensile: 2456.33 lbf/in^2
Sample 2 Elongation (350% Min): Pass
Sample 3 Median Thickness: 0.078
Sample 3 Thickness all Within 0.003 inch?: Yes
Sample 3 Ultimate Tensile: 2336.2 lbf/in^2
Sample 3 Elongation (350% Min): Pass
Median of the Ultimate Tensile Values: 2456.3 lbf/in^2
General comments (publicly viewable) (Max 1000 characters):
Test Graph
Source: Bluehill Data Point File
Test graph for Sample 1

Source: Bluehill Data Point File
Test graph for Sample 2

Source: Bluehill Data Point File
Test graph for Sample 3

Test was verified on 10/20/2020