Test 2020-06-03-8-4 (ASTM D624-00-re12) Summary

Project Information
Project IdentifiersProject ID: 210673
DEA: 042640F4
EFIS: 0400020132
COOP: 042308A3
DIST-CO-RTE-PM04-SON-101-4.0/7.1
Work DescriptionDESIGN THE NORTHERLY SEGMENT OF THE MARIN-SONOMA NARROWS PROJECT AND INCLUDES SOUND WALLS, BRIDGES, MEDIAN WIDENING AND RAMP WIDENING.
Location DescriptionJUST NORTH OF THE U.S. 101 AND STATE ROUTE 116 CONNECTION TO 0.3 MILE NORTH OF THE CORONA ROAD OVERCROSSING IN THE CITY OF PETALUMA.
Sample Information
Sample Taken Date6/3/2020 Sample Unique Key8
Will the laboratory/organization for which you are a member perform testing on this material sample?Yes Date that the sample was received by the laboratory/organization performing the testing6/5/2020
Sample typeQuality Assurance A brief description of the samplebearing pad
The quantity of what the sample constitutes2 From where was the sample collectedManufacturer
First name of sampler or witnessed byBrad Last name of sampler or witnessed byStreeter
Title of sampler Laboratory sample identification
The fabricator/manufacturer/facility nameScougal Rubber Transportation Laboratory (TL) Number
Inspector Lot Number from the Transportation Laboratory (TL) Form Structure unique identifier
Structure name
Material Information
Material TypeSMTL TM1 - Elastomeric Bearing Pad Mfg. Lot Number(s)18728-6
Material/Compound/Elastomer IDna Samples Representing62
Description (size)1"x4"x6" CommentsUnknown
Description (Number of Shims)2 Type of Bearing PadSteel
Description (Thickness of Shims)14 gage Manufacturer(s)Scougal Rubber
Batch Numberna
Test Details
DIME Sample ID: 2020-06-03-8
DIME Test ID: 2020-06-03-8-4
Testing Lab: CT HQ - Sacramento Structural Materials Testing Laboratory
Test Method: ASTM D624-00-re12: Standard Test Method for Tear Strength of Conventional Vulcanized Rubber and Thermoplastic Elastomers
Test Release Date: 2020-06-11
Test Results

Number of specimens tested: 3
Input Type: Measured
Tester's full name: spaine
Date of test: 06/10/2020
Humidity: 50.00 %
Temperature: 72 F
Sample 1 Median Thickness: 0.069
Sample 1 Tear Strength: 226.8
Sample 2 Median Thickness: 0.064
Sample 2 Tear Strength: 225.5
Sample 3 Median Thickness: 0.058
Sample 3 Tear Strength: 237.2
UTM:2kip
Median of the Tear Strength Values:226.8 lb/in
General comments (publicly viewable) (Max 250 characters):
Test Graph
Source: Bluehill Data Point File
Test graph for Sample 1

Source: Bluehill Data Point File
Test graph for Sample 2

Source: Bluehill Data Point File
Test graph for Sample 3

Test was verified on 06/11/2020