Summary for Test 2017-07-21-3-3

Test performed: ASTM D624-00-re12

Project Information

Project IdentifiersProject ID: 212253
DEA: 010H0304
EFIS: 0117000087
DIST-CO-RTE-PM01-HUM-96-20.0/24.0, 0.83
Award Date02/22/2017
Closeout Date01/08/2019
Work DescriptionREPAIR SLIPOUT
Location DescriptionIN HUMBOLDT COUNTY NEAR WEITCHPEC FROM 3.0 MILES OF KLAMATH RIVER BRIDGE #04-0144 TO 0.6 MILE EAST OF WEITCHPEC ROAD
QA Service Level1 (Verified on 04/24/2017)

Sample Information

Sample Taken Date07/21/2017 Sample Unique Key3
Date that the sample was received by the laboratory/organization performing the testing07/24/2017 Sample typeQuality Assurance
A brief description of the sample1 x 8 x 12 reinforced bearing pad The quantity of what the sample constitutes1 lot of 43
From where was the sample collectedManufacturer First name of sampler or witnessed byStacey
Last name of sampler or witnessed byDavis Title of samplerQAI
Telephone number of sampler5624806904 Laboratory sample identification
Linked DIME Sample ID The fabricator/manufacturer/facility nameCal-Neva
Transportation Laboratory (TL) Number Inspector Lot Number from the Transportation Laboratory (TL) FormB362-075-17
Structure unique identifierNot set Structure nameNot set
Bid ItemNot set

Material Information

Material TypeSMTL TM1 - Elastomeric Bearing Pad Mfg. Lot Number(s)N/A Heat 811V04180
Material/Compound/Elastomer IDRL305502 Samples Representing1 lot of 43
Description (size)1 x 8 12 Comments
Description (Number of Shims)2 Type of Bearing PadSteel
Description (Thickness of Shims)14 gage Manufacturer(s)Arcelormittal
Batch Number071017

Test Details

DIME Sample ID: 2017-07-21-3
DIME Test ID: 2017-07-21-3-3
Testing Lab: CT HQ - Sacramento Structural Materials Testing Laboratory
Test Method: ASTM D624-00-re12: Standard Test Method for Tear Strength of Conventional Vulcanized Rubber and Thermoplastic Elastomers
Test Release Date: 2017-08-07

Test Results


Number of specimens tested: 5
Input Type: Measured
Tester's full name: Brian
Date of test: 07/25/2017
Humidity: 50 %
Temperature: 72 F
Sample 1 Median Thickness: 0.08 in
Sample 1 Tear Strength: 175 lbf / in
Sample 2 Median Thickness: 0.066 in
Sample 2 Tear Strength: 227.3 lbf / in
Sample 3 Median Thickness: 0.075 in
Sample 3 Tear Strength: 240 lbf / in
Sample 4 Median Thickness: 0.077 in
Sample 4 Tear Strength: 233.8 lbf / in
Sample 5 Median Thickness: 0.072 in
Sample 5 Tear Strength: 236.1 lbf / in
UTM: no data
Median of the Tear Strength Values: 233.8 lb/in
General comments (publicly viewable) (Max 1000 characters):
Test Graph
Source: Partner Data Point File
Test graph for Sample 1

Source: Partner Data Point File
Test graph for Sample 2

Source: Partner Data Point File
Test graph for Sample 3

Source: Partner Data Point File
Test graph for Sample 4

Source: Partner Data Point File
Test graph for Sample 5

Test was verified on 7/31/2017 ✔