Summary for Test 2023-03-08-46-3

Test performed: ASTM D624-00r20

Project Information

Project IdentifiersProject ID: 994408
DEA: 051K03U4
EFIS: 0522000026
DIST-CO-RTE-PM05-SLO-101-10.02/10.5
Award Date10/04/2022
Closeout DateNot set
Work Description!!PLEASE CC Office Engineer Barbara Riccardi on reports to RE and SR!! Construct 2 roundabouts in Montecito along US 101.
Location DescriptionNot set
QA Service Level1 (Verified on 12/29/2022)

Sample Information

Sample Taken Date03/08/2023 Sample Unique Key46
Date that the sample was received by the laboratory/organization performing the testing03/13/2023 Sample typeQuality Assurance
A brief description of the sample1.15x4x6" LAM PAD w2 14ga SHIMS The quantity of what the sample constitutes9
From where was the sample collectedManufacturer First name of sampler or witnessed byBrad
Last name of sampler or witnessed byStreeter Title of sampler
Telephone number of sampler Laboratory sample identification
Linked DIME Sample ID The fabricator/manufacturer/facility nameScougal Rubber
Transportation Laboratory (TL) Number Inspector Lot Number from the Transportation Laboratory (TL) Form
Structure unique identifier Structure name
Bid ItemNot set

Material Information

Material TypeSMTL TM1 - Elastomeric Bearing Pad Mfg. Lot Number(s)22802-1-2
Material/Compound/Elastomer IDNA Samples Representing9
Description (size)1.15 x 4 x 6 Comments
Description (Number of Shims)2 Type of Bearing PadSteel
Description (Thickness of Shims)14 gage Manufacturer(s)Scougal Rubber
Batch NumberNA

Test Details

DIME Sample ID: 2023-03-08-46
DIME Test ID: 2023-03-08-46-3
Testing Lab: CT HQ - Sacramento Structural Materials Testing Laboratory
Test Method: ASTM D624-00r20: Standard Test Method for Tear Strength of Conventional Vulcanized Rubber and Thermoplastic Elastomers
Test Release Date: 2023-03-21

Test Results


Number of specimens tested: 5
Input Type: Measured
Tester's full name: aauvinen
Date of test: 03/17/2023
Humidity: 50.00 %
Temperature: 72 F
Sample 1 Median Thickness: 0.054
Sample 1 Tear Strength: 251.3
Sample 2 Median Thickness: 0.057
Sample 2 Tear Strength: 248
Sample 3 Median Thickness: 0.056
Sample 3 Tear Strength: 154.3
Sample 4 Median Thickness: 0.055
Sample 4 Tear Strength: 167.8
Sample 5 Median Thickness: 0.054
Sample 5 Tear Strength: 214.1
UTM: 2kip
Median of the Tear Strength Values: 214.1 lb/in
General comments (publicly viewable) (Max 1000 characters):
Test Graph
Source: Bluehill Data Point File
Test graph for Sample 5

Source: Bluehill Data Point File
Test graph for Sample 3

Source: Bluehill Data Point File
Test graph for Sample 1

Source: Bluehill Data Point File
Test graph for Sample 4

Source: Bluehill Data Point File
Test graph for Sample 2

Test was verified on 3/21/2023 ✔