Summary for Test 2016-07-21-5-1

Test performed: CTM 670-December 2013

Project Information

Project IdentifiersProject ID: 210808
DEA: 020E0904
EFIS: 0200000016
DIST-CO-RTE-PM02-SHA-5-R29.3/R31.1,R45.0/R45.8
Award Date02/03/2016
Closeout Date10/21/2020
Work DescriptionREPLACE BRIDGE, REALIGN ROADWAY AND SEISMIC RETROFIT
Location DescriptionIN SHASTA COUNTY ABT 8 MI N OF SHASTA LAKE CTY AND NEAR LAKEHEAD FRM TURNTABLE BAY O/C TO 0.1 MI N OF O'BRIEN SRRA & FRM 0.4 MI S TO 0.3 MI N OF DOG CREEK BRIDGE.
QA Service Level1 (Verified on 09/23/2015)

Sample Information

Sample Taken Date07/21/2016 Sample Unique Key5
Date that the sample was received by the laboratory/organization performing the testing07/22/2016 Sample typeQuality Assurance
A brief description of the sampleFlash Welded Rebar Hoops The quantity of what the sample constitutes8
From where was the sample collectedFabricator First name of sampler or witnessed byED
Last name of sampler or witnessed byFleming Title of samplerUnknown
Telephone number of samplerUnknown Laboratory sample identificationUnknown
Linked DIME Sample IDUnknown The fabricator/manufacturer/facility nameHarris Rebar Nucor
Transportation Laboratory (TL) NumberC715253 Inspector Lot Number from the Transportation Laboratory (TL) FormB1029716
Structure unique identifierNot set Structure nameNot set
Bid ItemNot set

Material Information

Material TypeSMTL TM5 - Welded Hoops Production or Authorization TestingProduction Testing
Service or UltimateService Rebar Heat Number(s)SE12105674, SE16100880
Hoop Manufacturer Lot Number(s)H09, H10 Material Standard CodeASTM A706
Material Grade60 Rebar Size8
Diameter of Hoop7'-0" Epoxy CoatedNo
Epoxy Coating ColorNA Rebar ManufacturerNucor
Welding CompanyHarris Rebar Coating StandardsUncoated
Weld TypeFlash Welded

Test Details

DIME Sample ID: 2016-07-21-5
DIME Test ID: 2016-07-21-5-1
Testing Lab: CT HQ - Sacramento Structural Materials Testing Laboratory
Test Method: CTM 670-December 2013: Method of Tests for Mechanical and Welded Reinforcing Steel Splices (Tensile)
Test Release Date: 2016-07-26

Test Results


Number of Samples: 1
Input Type: Measured
Tester's full name: Fred
Date of test: 07/25/2016
UTM: 400KIP
Temperature: 72 F
NumSampleMfg. Lot Number(s)SizeArea (sqin)Peak Load (lbf)Peak Stress (psi)CommentsTested By
11H09#8/25mm0.797817098950Bar BrokeFred

General comments (publicly viewable) (Max 1000 characters): Bar Broke; OK Necking
Test Graph
Source: Partner Data Point File
Test graph for the Sample

Test was verified on 7/26/2016 ✔