Summary for Test 2021-09-02-26-3

Test performed: ASTM D5329-16

Project Information

Project IdentifiersProject ID: 215161
DEA: 010C5704
EFIS: 0113000009
DIST-CO-RTE-PM01-HUM-101-69.8/75.2
Award Date11/09/2020
Closeout Date04/04/2022
Work DescriptionPLACE RHMA-G, HMA AND CONCRETE BARRIER.
Location DescriptionHUMBOLDT COUNTY IN AND NEAR EUREKA FROM 0.8 MILE SOUTH OF TOMPKINS HILL ROAD OVERHEAD TO 0.4 MILE NORTH OF HERRICK AVENUE OVERCROSSING
QA Service Level1 (Verified on 09/15/2020)

Sample Information

Sample Taken Date09/02/2021 Sample Unique Key26
Date that the sample was received by the laboratory/organization performing the testing09/09/2021 Sample typeDepartment Acceptance
A brief description of the samplePG64-16 Rubber Blend The quantity of what the sample constitutes2 cans
From where was the sample collectedManufacturer First name of sampler or witnessed byJohn
Last name of sampler or witnessed byAtturo Title of sampler
Telephone number of sampler Laboratory sample identification
Linked DIME Sample ID The fabricator/manufacturer/facility nameMercer Fraser Plant B
Transportation Laboratory (TL) Numberc972623 Inspector Lot Number from the Transportation Laboratory (TL) Form
Structure unique identifier Structure name
Bid ItemNot set

Material Information

Material TypeAsphalt Rubber Binder Asphalt modifier supplier
Performance GradePG 64-16 Lot number
Sublot number Asphalt Rubber Binder Mix NumberNot set

Test Details

DIME Sample ID: 2021-09-02-26
DIME Test ID: 2021-09-02-26-3
Testing Lab: CT HQ - Sacramento Asphalt Binder Laboratory
Test Method: ASTM D5329-16: Standard Test Methods for Sealants and Fillers, Hot-Applied, for Joints and Cracks in Asphalt Pavements and Portland Cement Concrete Pavements (Asphalt Pavement)
Test Release Date: 2021-09-15

Test Results


Input Type: Measured
Tester's full name: Minoo Ahmadi
Date of test: 09/14/2021
Temperature: 25 C
Ball Penetration (P1): 1 mm
Final Dial reading (F1): 65 mm
Ball Penetration (P2): 1 mm
Final Dial reading (F2): 65 mm
Ball Penetration (P3): 1 mm
Final Dial reading (F3): 67 mm
Resilience 1: 36 %
Resilience 2: 36 %
Resilience 3: 34 %
Average Resilience: 35 %
Minutes Reaction: no data
General comments (publicly viewable) (Max 1000 characters): Per 2018 Standard Specifications

Test was verified on 9/15/2021 ✔