Summary for Test 2019-08-16-8-2

Test performed: AASHTO T283-14

Project Information

Project Identifiers
DEA: No Project
DIST-CO-RTE-PM---
Award DateNot set
Closeout Date11/01/2022
Work DescriptionSpecial project identifier for material not associated with a project
Location DescriptionNot set
QA Service LevelNOT VERIFIED

Sample Information

Sample Taken Date08/16/2019 Sample Unique Key8
Will the laboratory/organization for which you are a member perform testing on this material sample?No Date that the sample was received by the laboratory/organization performing the testing08/16/2019
Sample typeQuality Control A brief description of the sample1/2 HMA A
The quantity of what the sample constitutesJMF Verification From where was the sample collectedSource
First name of sampler or witnessed byCarlos Last name of sampler or witnessed byManzo
Title of samplerQC Technician Telephone number of sampler
Laboratory sample identificationTEM12SPLA Linked DIME Sample ID
The fabricator/manufacturer/facility nameSPM-Templeton Transportation Laboratory (TL) Number
Inspector Lot Number from the Transportation Laboratory (TL) Form Structure unique identifier
Structure name

Material Information

Material TypeHot Mix Asphalt HMA TypeType A HMA
HMA Grading1/2 inch Lot number
Sublot number HMA Mix NumberNot set

Test Details

DIME Sample ID: 2019-08-16-8
DIME Test ID: 2019-08-16-8-2
Testing Lab: Sierra Pacific Materials
Test Method: AASHTO T283-14: Standard Method of Test for Resistance of Compacted Asphalt Mixtures to Moisture-Induced Damage (Moisture Content)
Test Release Date: 2019-08-23

Test Results


Unit system used?: SI Units
Input Type: Calculated
Tester's full name: unknown
Date of test: 08/23/2019
Specimen Treatment: Treated
Average Dry Tensile Strength: 241 psi
Average Wet Tensile Strength: 198 psi
Tensile Strength Ratio: 82