Summary for Test 2019-01-09-2-2
Test performed: ASTM C109-11Project Information
Project Identifiers | Project ID: 8801 DEA: AML-CEM EFIS: AML-CEM |
---|---|
DIST-CO-RTE-PM | 59--- |
Award Date | Not set |
Closeout Date | Not set |
Work Description | Special project for Cementitious Materials for use in Concrete Authorized Material List (AML) |
Location Description | Not set |
QA Service Level | NOT VERIFIED |
Sample Information
Sample Taken Date | 01/09/2019 | Sample Unique Key | 2 |
---|---|---|---|
Will the laboratory/organization for which you are a member perform testing on this material sample? | Yes | Date that the sample was received by the laboratory/organization performing the testing | 01/09/2019 |
Sample type | Annual Source Testing | A brief description of the sample | Slag Cement NewCem |
The quantity of what the sample constitutes | 1 Bucket | From where was the sample collected | Source |
First name of sampler or witnessed by | Unknown | Last name of sampler or witnessed by | Unknown |
Title of sampler | Unknown | Telephone number of sampler | Unknown |
Laboratory sample identification | CM195905 | Linked DIME Sample ID | Unknown |
The fabricator/manufacturer/facility name | LaFarge | Transportation Laboratory (TL) Number | Unknown |
Inspector Lot Number from the Transportation Laboratory (TL) Form | Unknown | Structure unique identifier | Not set |
Structure name | Not set |
Material Information
Material Type | Cementitious | Brand | LaFarge |
---|---|---|---|
Mill | Seattle | Type of Cementitious Material | Slag Cement |
Test Details
DIME Sample ID: 2019-01-09-2
DIME Test ID: 2019-01-09-2-2
Testing Lab: CT HQ - Sacramento Cement Testing Laboratory
Test Method: ASTM C109-11: Compressive Strength of Hydraulic Cement Mortars (Using 2-in. or [50mm] Cube Specimens)
Test Release Date: 2021-01-22
Test Results
Will control cubes be used per ASTM C311?: yes
Input Type: Measured
Tester's full name: SA
Date of test: 05/16/2019
Age of specimen: 7 days
The amount of flow (In percent): 109 %
The amount of water used (In percent): 48.2 %
Maximum load of 1st specimen (lb): 12013 lb
Maximum load of 2nd specimen (lb): 11726 lb
Maximum load of 3rd specimen (lb): 12817 lb
Cross sectional area loaded of 1st specimen (sq. inch): 4 in^2
Cross sectional area loaded of 2nd specimen (sq. inch): 4 in^2
Cross sectional area loaded of 3rd specimen (sq. inch): 4 in^2
Average Compressive strength (to nearest 10 psi) control group: 4560 psi
Compressive strength of 1st specimen (psi): 3003 psi
Compressive strength of 2nd specimen (psi): 2932 psi
Compressive strength of 3rd specimen (psi): 3204 psi
Average Compressive strength (to nearest 10 psi): 3050 psi
Strength Activity Index of Portland Cement per ASTM C311: 67
General comments (publicly viewable) (Max 1000 characters): 7 Day Break. Should have thrown out third cube making average 2970 psi and Strength Activity Index 65%.
Test Graph
Source: Partner Data Point FileTest graph for Specimen 1 of 3
Source: Partner Data Point File
Test graph for Specimen 2 of 3
Source: Partner Data Point File
Test graph for Specimen 3 of 3
Test was verified on 1/22/2021 ✔