Summary for Test 2018-03-13-10-3

Test performed: ASTM D624-00-re12

Project Information

Project IdentifiersProject ID: 210569
DEA: 083555V4
EFIS: 0814000086
DIST-CO-RTE-PM08-SBD-15-42.5/46.0
Award Date11/05/2015
Closeout Date01/18/2022
Work DescriptionWIDEN I-15, RECONSTRUCT 3 IC'S, CONSTRUCT 2 NEW BR AND WIDEN 3 BR.
Location DescriptionSAN BERNARDINO COUNTY IN VICTORVILLE FROM 0.5 MILE NORTH OF MOJAVE DRIVE TO 1.5 MILE NORTH OF STODDARD WELLS ROAD OVERCROSSING
QA Service Level1 (Verified on 10/15/2015)

Sample Information

Sample Taken Date03/13/2018 Sample Unique Key10
Will the laboratory/organization for which you are a member perform testing on this material sample?Yes Date that the sample was received by the laboratory/organization performing the testing03/15/2018
Sample typeQuality Assurance A brief description of the sampleBearing Pad
The quantity of what the sample constitutes1 From where was the sample collectedManufacturer
First name of sampler or witnessed byPet Last name of sampler or witnessed byEtcheverry
Title of samplerUnknown Telephone number of samplerUnknown
Laboratory sample identificationUnknown Linked DIME Sample IDUnknown
The fabricator/manufacturer/facility nameScougal Rubber Transportation Laboratory (TL) NumberUnknown
Inspector Lot Number from the Transportation Laboratory (TL) FormUnknown Structure unique identifierNot set
Structure nameNot set

Material Information

Material TypeSMTL TM1 - Elastomeric Bearing Pad Mfg. Lot Number(s)16318-1R
Material/Compound/Elastomer IDUnknown Samples Representing11
Description (size)5"x15"x15" CommentsUnknown
Description (Number of Shims)10 Type of Bearing PadSteel
Description (Thickness of Shims)14 gage Manufacturer(s)Scougal Rubber
Batch NumberUnknown

Test Details

DIME Sample ID: 2018-03-13-10
DIME Test ID: 2018-03-13-10-3
Testing Lab: CT HQ - Sacramento Structural Materials Testing Laboratory
Test Method: ASTM D624-00-re12: Standard Test Method for Tear Strength of Conventional Vulcanized Rubber and Thermoplastic Elastomers
Test Release Date: 2018-04-02

Test Results


Number of specimens tested: 5
Input Type: Measured
Tester's full name: Randy
Date of test: 03/19/2018
Humidity: 50 %
Temperature: 70 F
Sample 1 Median Thickness: 0.067 in
Sample 1 Tear Strength: 179.1 lbf / in
Sample 2 Median Thickness: 0.062 in
Sample 2 Tear Strength: 177.4 lbf / in
Sample 3 Median Thickness: 0.067 in
Sample 3 Tear Strength: 223.9 lbf / in
Sample 4 Median Thickness: 0.06 in
Sample 4 Tear Strength: 216.7 lbf / in
Sample 5 Median Thickness: 0.064 in
Sample 5 Tear Strength: 187.5 lbf / in
UTM: no data
Median of the Tear Strength Values: 187.5 lb/in
General comments (publicly viewable) (Max 1000 characters):
Test Graph
Source: Partner Data Point File
Test graph for Sample 3

Source: Partner Data Point File
Test graph for Sample 1

Source: Partner Data Point File
Test graph for Sample 2

Source: Partner Data Point File
Test graph for Sample 4

Source: Partner Data Point File
Test graph for Sample 5

Test was verified on 3/26/2018