Summary for Test 2017-01-24-2-2
Test performed: ASTM D412-06a-re13Project Information
Project Identifiers | Project ID: 211668 DEA: 010B2604 EFIS: 0112000150 |
---|---|
DIST-CO-RTE-PM | 01-DN-199-8.2 |
Award Date | 11/07/2016 |
Closeout Date | 01/07/2019 |
Work Description | CONSTRUCT BRIDGE AND WIDEN SHOULDERS |
Location Description | DEL NORTE COUNTY NEAR HIOUCHI AT 1 MILE NORTH OF SOUTH FORK ROAD |
QA Service Level | 1 (Verified on 09/27/2016) |
Sample Information
Sample Taken Date | 01/24/2017 | Sample Unique Key | 2 |
---|---|---|---|
Will the laboratory/organization for which you are a member perform testing on this material sample? | Yes | Date that the sample was received by the laboratory/organization performing the testing | 01/24/2017 |
Sample type | Quality Assurance | A brief description of the sample | Bearing Pad |
The quantity of what the sample constitutes | 2 | From where was the sample collected | Manufacturer |
First name of sampler or witnessed by | Rob | Last name of sampler or witnessed by | Anderson |
Title of sampler | Unknown | Telephone number of sampler | Unknown |
Laboratory sample identification | Unknown | Linked DIME Sample ID | Unknown |
The fabricator/manufacturer/facility name | Scougal Rubber | Transportation Laboratory (TL) Number | NA |
Inspector Lot Number from the Transportation Laboratory (TL) Form | NA | Structure unique identifier | Not set |
Structure name | Not set |
Material Information
Material Type | SMTL TM1 - Elastomeric Bearing Pad | Mfg. Lot Number(s) | 15480-1,2 |
---|---|---|---|
Material/Compound/Elastomer ID | NA | Samples Representing | 2 |
Description (size) | 3" x 12" x 12" | Comments | Unknown |
Description (Number of Shims) | 6 | Type of Bearing Pad | Steel |
Description (Thickness of Shims) | 14 gage | Manufacturer(s) | Scougal Rubber |
Batch Number | NA |
Test Details
DIME Sample ID: 2017-01-24-2
DIME Test ID: 2017-01-24-2-2
Testing Lab: CT HQ - Sacramento Structural Materials Testing Laboratory
Test Method: ASTM D412-06a-re13: Standard Test Methods for Vulcanized Rubber and Thermoplastic Elastomers-Tension
Test Release Date: 2017-02-09
Test Results
Number of specimens tested: 3
Unit of the Ultimate Tensile Values: lbf per sqr in
Input Type: Calculated
Tester's full name: Brian
Date of test: 01/27/2017
UTM: 2KIP
Humidity: 50 %
Temperature: 72 F
Sample 1 Median Thickness: 0.081 in
Sample 1 Thickness all Within 0.003 inch?: Yes
Sample 1 Ultimate Tensile: 3054.2 lbf/in^2
Sample 1 Elongation (350% Min): Pass
Sample 2 Median Thickness: 0.079 in
Sample 2 Thickness all Within 0.003 inch?: Yes
Sample 2 Ultimate Tensile: 2676.8 lbf/in^2
Sample 2 Elongation (350% Min): Pass
Sample 3 Median Thickness: 0.076 in
Sample 3 Thickness all Within 0.003 inch?: Yes
Sample 3 Ultimate Tensile: 3052.6 lbf/in^2
Sample 3 Elongation (350% Min): Pass
Median of the Ultimate Tensile Values: 3052.6 lbf/in^2
General comments (publicly viewable) (Max 1000 characters):
Test Graph
Source: Partner Data Point FileTest graph for Sample 1
Source: Partner Data Point File
Test graph for Sample 2
Source: Partner Data Point File
Test graph for Sample 3
Test was verified on 2/2/2017 ✔