Unit system used? | US Units |
Number of specimens | 2 |
Test performed | With no density determined |
Cross sectional area of cylinder 1 | 28.46 in^2 |
Cross sectional area of cylinder 2 | 28.46 in^2 |
Capped in accordance with? | ASTM C617/CTM521 |
Compressive strength (to nearest 10 psi) | 2810 psi |
Average diameter of cylinder 1 | 6.02 in |
Average diameter of cylinder 2 | 6.02 in |
Compressive strength of cylinder 1 | 2761.8 psi |
Compressive strength of cylinder 2 | 2865.8 psi |
Maximum load on cylinder 1 | 78600 lb |
Maximum load on cylinder 2 | 81560 lb |
Type of fracture pattern of cylinder 1 | 1 |
Type of fracture pattern of cylinder 2 | 1 |
Comment on any defect in either specimen or caps (Max 250 Characters) | no data |
Correction factor for cylinder 1 | 1 |
Correction factor for cylinder 2 | no data |
Age of specimen | 7 days |
Unit system used? | US Units |
Number of specimens | 2 |
Test performed | With no density determined |
Cross sectional area of cylinder 1 | 28.27 in^2 |
Cross sectional area of cylinder 2 | 28.27 in^2 |
Capped in accordance with? | ASTM C617/CTM521 |
Compressive strength (to nearest 10 psi) | 3590 psi |
Average diameter of cylinder 1 | 6.00 in |
Average diameter of cylinder 2 | 6.00 in |
Compressive strength of cylinder 1 | 3637.4 psi |
Compressive strength of cylinder 2 | 3551.5 psi |
Maximum load on cylinder 1 | 102830 lb |
Maximum load on cylinder 2 | 100400 lb |
Type of fracture pattern of cylinder 1 | 1 |
Type of fracture pattern of cylinder 2 | 1 |
Comment on any defect in either specimen or caps (Max 250 Characters) | no data |
Correction factor for cylinder 1 | 1 |
Correction factor for cylinder 2 | no data |
Age of specimen | 28 days |