Print Report | Back to Test Summary

Testing Report for 2016-09-15-5-3

Note: Fields with no data or with a value of "Unknown" will not be displayed on the print out.

Project Information

DEA: 59912684
EFIS:
Project ID: 8196
QA Service Level: 1
DIST-CO-RTE-PM: 59---
Work Description:
Location Description:
Contractor Name: Unknown
Contractor Address: Unknown
Resident Engineer: Unknown
Structure Rep.: Unknown

Sample Information

DIME Sample ID: 2016-09-15-5
TL Number from the TL Form: NA
Sample Submitted By Organization: CT HQ - Sacramento Structural Materials Testing Laboratory
Sample Organization Contact: (916) 227-7253
Type of Sample: Quality Assurance
Type of Material: SMTL TM1 - Elastomeric Bearing Pad
Sample Taken Date: 9/15/2016
Date that the sample was received by the laboratory/organization performing the testing: 9/20/2016
The quantity of what the sample constitutes: 1
A brief description of the sample: Bearing Pad
From where was the sample collected: Source
Laboratory sample identification: Unknown
Structure unique identifier:
Structure name:
The fabricator/manufacturer/facility name: DynaTech

Material Information

Mfg. Lot Number(s): 082416
Material/Compound/Elastomer ID: NA
Samples Representing: 1
Description (size): 70mm x 179mm x 320mm
Comments: Unknown
Description (Number of Shims): 3
Type of Bearing Pad: Steel
Description (Thickness of Shims): NA
Manufacturer(s): DynaTech
Batch Number: NA

Test Information

DIME Test ID: 2016-09-15-5-3
Test Method: ASTM D624-00-re12: Standard Test Method for Tear Strength of Conventional Vulcanized Rubber and Thermoplastic Elastomers
Date Tested: 9/21/2016
Verified Date: 9/26/2016
Submitted By Organization: CT HQ - Sacramento Structural Materials Testing Laboratory
Organization Address: 5900 Folsom Blvd,
Organization City: Sacramento
Organization State: CA
Organization Zipcode: 95819
Organization Email: paul.lukkarila@dot.ca.gov
Organization Phone: (916) 227-7253
General Comments for this Test:
Test Result Compliance:
Additional Comments When Verified :

Submitted Test Results

Number of specimens tested: 3
UTM: no data
Humidity: 50 %
Temperature: 72 F
Sample 1 Median Thickness: 0.072 in
Sample 1 Tear Strength: 277.8 lbf / in
Sample 2 Median Thickness: 0.071 in
Sample 2 Tear Strength: 239.4 lbf / in
Sample 3 Median Thickness: 0.074 in
Sample 3 Tear Strength: 229.7 lbf / in
Median of the Tear Strength Values: 239.4 lb/in