Note: Fields with no data or with a value of "Unknown" will not be displayed on the print out.
Project ID: 214697 DEA: 07307104 EFIS: 0714000213
QA Service Level: 1
DIST-CO-RTE-PM: 07-LA-101-32.8
Work Description: CONSTRUCT BRIDGE.
Location Description: LOS ANGELES COUNTY IN AND NEAR AGOURA HILLS FROM 0.1 MILE WEST OF LIBERTY CANYON ROAD UNDERCROSSING TO 0.6 MILE EAST OF PALO COMADO OVERCROSSING
Contractor Name: CA Rasmussen
Contractor Address: 28548 LIVINGSTON AVENUE, VALENICA CA 91355
Resident Engineer: Sam Toutounchian Structure Rep.: Darwin Vargas
DIME Sample ID: 2024-06-22-6
TL Number from the TL Form: 062224
Sample Submitted By Organization: CT D07 - Materials Field Laboratory, Unit 1953
Sample Organization Contact: (213) 817-0387
Type of Sample: Acceptance
Type of Material: Concrete
Sample Taken Date: 06/22/2024
Date that the sample was received by the laboratory/organization performing the testing: 06/24/2024
The quantity of what the sample constitutes: 130 CY
A brief description of the sample: 4X8 PCC cylinders
From where was the sample collected: Job Site
Laboratory sample identification: 24-161
Structure unique identifier:
Structure name:
The fabricator/manufacturer/facility name: National Ready Mix Concrete Company
The concrete mix design number: S72C443T1U
The truck number from where the sample was collected: 31
The batch plant ticket number from where the sample was collected: 726918
Concrete batch plant: National Ready Mix Concrete Canoga
The fabricator/manufacturer designation for the sample:
A detailed description of where the material sample was collected: truck chute
Where the material sample would have been placed if not sampled:
From Lot No.:
Bag Lot No.:
DIME Test ID: 2024-06-22-6-1
Test Method: CTM 521-June 2020: Method of Test for Compressive Strength of Molded Concrete Cylinders
Verified Date: 06/26/2024
Date Tested: 06/25/2024
Submitted By Organization: CT D07 - Materials Field Laboratory, Unit 1953
Organization Address: 1940 South Workman Mill Road,
Organization City: Whittier
Organization State: CA
Organization Zipcode: 90601
Organization Email: chad.chotibhongs@dot.ca.gov
Organization Phone: (213) 817-0387
General Comments for this Test:
Test Result Compliance: not applicable
Additional Comments When Verified:
Unit system used?
|
US Units
|
Number of specimens
|
3
|
Test performed
|
With no density determined
|
Capped in accordance with?
|
ASTM C617 - Sulfur Mortar Cap
|
Average diameter of cylinder 1
|
4.01 in
|
Average diameter of cylinder 2
|
4.01 in
|
Average diameter of cylinder 3
|
4.02 in
|
Cross sectional area of cylinder 1
|
12.63 in^2
|
Cross sectional area of cylinder 2
|
12.63 in^2
|
Cross sectional area of cylinder 3
|
12.69 in^2
|
Compressive strength (to nearest 10 psi)
|
2960 psi
|
Maximum load on cylinder 1
|
37842 lb
|
Maximum load on cylinder 2
|
37078 lb
|
Maximum load on cylinder 3
|
37556 lb
|
Compressive strength of cylinder 1
|
2,996.2 psi
|
Type of fracture pattern of cylinder 1
|
2
|
Compressive strength of cylinder 2
|
2,935.7 psi
|
Compressive strength of cylinder 3
|
2,959.5 psi
|
Type of fracture pattern of cylinder 2
|
2
|
Type of fracture pattern of cylinder 3
|
2
|
Comment on any defect in either specimen or caps (Max 250 Characters)
|
no data
|
Correction factor for cylinder 1
|
1.00
|
Correction factor for cylinder 2
|
1.00
|
Correction factor for cylinder 3
|
1.00
|
Age of specimen
|
3 days
|
Age of specimen in hours
|
no data0 hours
|
DIME Test ID: 2024-06-22-6-2
Test Method: CTM 521-June 2020: Method of Test for Compressive Strength of Molded Concrete Cylinders
Verified Date: 07/01/2024
Date Tested: 06/29/2024
Submitted By Organization: CT D07 - Materials Field Laboratory, Unit 1953
Organization Address: 1940 South Workman Mill Road,
Organization City: Whittier
Organization State: CA
Organization Zipcode: 90601
Organization Email: chad.chotibhongs@dot.ca.gov
Organization Phone: (213) 817-0387
General Comments for this Test:
Test Result Compliance: not applicable
Additional Comments When Verified:
Unit system used?
|
US Units
|
Number of specimens
|
3
|
Test performed
|
With no density determined
|
Capped in accordance with?
|
ASTM C617 - Sulfur Mortar Cap
|
Average diameter of cylinder 1
|
4.01 in
|
Average diameter of cylinder 2
|
4.00 in
|
Average diameter of cylinder 3
|
4.00 in
|
Cross sectional area of cylinder 1
|
12.63 in^2
|
Cross sectional area of cylinder 2
|
12.57 in^2
|
Cross sectional area of cylinder 3
|
12.57 in^2
|
Compressive strength (to nearest 10 psi)
|
3500 psi
|
Maximum load on cylinder 1
|
44947 lb
|
Maximum load on cylinder 2
|
43727 lb
|
Maximum load on cylinder 3
|
43701 lb
|
Compressive strength of cylinder 1
|
3,558.7 psi
|
Type of fracture pattern of cylinder 1
|
2
|
Compressive strength of cylinder 2
|
3,478.7 psi
|
Compressive strength of cylinder 3
|
3,476.6 psi
|
Type of fracture pattern of cylinder 2
|
2
|
Type of fracture pattern of cylinder 3
|
2
|
Comment on any defect in either specimen or caps (Max 250 Characters)
|
no data
|
Correction factor for cylinder 1
|
1.00
|
Correction factor for cylinder 2
|
1.00
|
Correction factor for cylinder 3
|
1.00
|
Age of specimen
|
7 days
|
Age of specimen in hours
|
no data0 hours
|
DIME Test ID: 2024-06-22-6-3
Test Method: CTM 521-June 2020: Method of Test for Compressive Strength of Molded Concrete Cylinders
Verified Date: 07/10/2024
Date Tested: 07/10/2024
Submitted By Organization: CT D07 - Materials Field Laboratory, Unit 1953
Organization Address: 1940 South Workman Mill Road,
Organization City: Whittier
Organization State: CA
Organization Zipcode: 90601
Organization Email: chad.chotibhongs@dot.ca.gov
Organization Phone: (213) 817-0387
General Comments for this Test:
Test Result Compliance: complies
Additional Comments When Verified:
Unit system used?
|
US Units
|
Number of specimens
|
3
|
Test performed
|
With no density determined
|
Capped in accordance with?
|
ASTM C617 - Sulfur Mortar Cap
|
Average diameter of cylinder 1
|
4.00 in
|
Average diameter of cylinder 2
|
4.01 in
|
Average diameter of cylinder 3
|
4.00 in
|
Cross sectional area of cylinder 1
|
12.57 in^2
|
Cross sectional area of cylinder 2
|
12.63 in^2
|
Cross sectional area of cylinder 3
|
12.57 in^2
|
Compressive strength (to nearest 10 psi)
|
4400 psi
|
Maximum load on cylinder 1
|
57458 lb
|
Maximum load on cylinder 2
|
53524 lb
|
Maximum load on cylinder 3
|
55375 lb
|
Compressive strength of cylinder 1
|
4,571.0 psi
|
Type of fracture pattern of cylinder 1
|
2
|
Compressive strength of cylinder 2
|
4,237.8 psi
|
Compressive strength of cylinder 3
|
4,405.3 psi
|
Type of fracture pattern of cylinder 2
|
2
|
Type of fracture pattern of cylinder 3
|
2
|
Comment on any defect in either specimen or caps (Max 250 Characters)
|
no data
|
Correction factor for cylinder 1
|
1.00
|
Correction factor for cylinder 2
|
1.00
|
Correction factor for cylinder 3
|
1.00
|
Age of specimen
|
18 days
|
Age of specimen in hours
|
no data0 hours
|
DIME Test ID: 2024-06-22-6-4
Test Method: CTM 521-June 2020: Method of Test for Compressive Strength of Molded Concrete Cylinders
Verified Date: 08/05/2024
Date Tested: 07/20/2024
Submitted By Organization: CT D07 - Materials Field Laboratory, Unit 1953
Organization Address: 1940 South Workman Mill Road,
Organization City: Whittier
Organization State: CA
Organization Zipcode: 90601
Organization Email: chad.chotibhongs@dot.ca.gov
Organization Phone: (213) 817-0387
General Comments for this Test:
Test Result Compliance: complies
Additional Comments When Verified:
Unit system used?
|
US Units
|
Number of specimens
|
3
|
Test performed
|
With no density determined
|
Capped in accordance with?
|
ASTM C617 - Sulfur Mortar Cap
|
Average diameter of cylinder 1
|
4.01 in
|
Average diameter of cylinder 2
|
4.01 in
|
Average diameter of cylinder 3
|
4.02 in
|
Cross sectional area of cylinder 1
|
12.63 in^2
|
Cross sectional area of cylinder 2
|
12.63 in^2
|
Cross sectional area of cylinder 3
|
12.69 in^2
|
Compressive strength (to nearest 10 psi)
|
4930 psi
|
Maximum load on cylinder 1
|
61262 lb
|
Maximum load on cylinder 2
|
63270 lb
|
Maximum load on cylinder 3
|
62386 lb
|
Compressive strength of cylinder 1
|
4,850.5 psi
|
Type of fracture pattern of cylinder 1
|
2
|
Compressive strength of cylinder 2
|
5,009.5 psi
|
Compressive strength of cylinder 3
|
4,916.2 psi
|
Type of fracture pattern of cylinder 2
|
2
|
Type of fracture pattern of cylinder 3
|
2
|
Comment on any defect in either specimen or caps (Max 250 Characters)
|
no data
|
Correction factor for cylinder 1
|
1.00
|
Correction factor for cylinder 2
|
1.00
|
Correction factor for cylinder 3
|
1.00
|
Age of specimen
|
28 days
|
Age of specimen in hours
|
no data0 hours
|
DIME Test ID: 2024-06-22-6-5
Test Method: CTM 521-June 2020: Method of Test for Compressive Strength of Molded Concrete Cylinders
Verified Date: 08/05/2024
Date Tested: 08/03/2024
Submitted By Organization: CT D07 - Materials Field Laboratory, Unit 1953
Organization Address: 1940 South Workman Mill Road,
Organization City: Whittier
Organization State: CA
Organization Zipcode: 90601
Organization Email: chad.chotibhongs@dot.ca.gov
Organization Phone: (213) 817-0387
General Comments for this Test:
Test Result Compliance: complies
Additional Comments When Verified:
Unit system used?
|
US Units
|
Number of specimens
|
3
|
Test performed
|
With no density determined
|
Capped in accordance with?
|
ASTM C617 - Sulfur Mortar Cap
|
Average diameter of cylinder 1
|
4.02 in
|
Average diameter of cylinder 2
|
4.01 in
|
Average diameter of cylinder 3
|
4.00 in
|
Cross sectional area of cylinder 1
|
12.69 in^2
|
Cross sectional area of cylinder 2
|
12.63 in^2
|
Cross sectional area of cylinder 3
|
12.57 in^2
|
Compressive strength (to nearest 10 psi)
|
5520 psi
|
Maximum load on cylinder 1
|
71317 lb
|
Maximum load on cylinder 2
|
68150 lb
|
Maximum load on cylinder 3
|
69634 lb
|
Compressive strength of cylinder 1
|
5,619.9 psi
|
Type of fracture pattern of cylinder 1
|
2
|
Compressive strength of cylinder 2
|
5,395.9 psi
|
Compressive strength of cylinder 3
|
5,539.7 psi
|
Type of fracture pattern of cylinder 2
|
2
|
Type of fracture pattern of cylinder 3
|
2
|
Comment on any defect in either specimen or caps (Max 250 Characters)
|
no data
|
Correction factor for cylinder 1
|
1.00
|
Correction factor for cylinder 2
|
1.00
|
Correction factor for cylinder 3
|
1.00
|
Age of specimen
|
42 days
|
Age of specimen in hours
|
no data0 hours
|
DIME Test ID: 2024-06-22-6-6
Test Method: CTM 521-June 2020: Method of Test for Compressive Strength of Molded Concrete Cylinders
Verified Date: 08/19/2024
Date Tested: 08/17/2024
Submitted By Organization: CT D07 - Materials Field Laboratory, Unit 1953
Organization Address: 1940 South Workman Mill Road,
Organization City: Whittier
Organization State: CA
Organization Zipcode: 90601
Organization Email: chad.chotibhongs@dot.ca.gov
Organization Phone: (213) 817-0387
General Comments for this Test:
Test Result Compliance: complies
Additional Comments When Verified:
Unit system used?
|
US Units
|
Number of specimens
|
3
|
Test performed
|
With no density determined
|
Capped in accordance with?
|
ASTM C617 - Sulfur Mortar Cap
|
Average diameter of cylinder 1
|
4.01 in
|
Average diameter of cylinder 2
|
4.02 in
|
Average diameter of cylinder 3
|
4.01 in
|
Cross sectional area of cylinder 1
|
12.63 in^2
|
Cross sectional area of cylinder 2
|
12.69 in^2
|
Cross sectional area of cylinder 3
|
12.63 in^2
|
Compressive strength (to nearest 10 psi)
|
5890 psi
|
Maximum load on cylinder 1
|
74116 lb
|
Maximum load on cylinder 2
|
74857 lb
|
Maximum load on cylinder 3
|
74456 lb
|
Compressive strength of cylinder 1
|
5,868.3 psi
|
Type of fracture pattern of cylinder 1
|
2
|
Compressive strength of cylinder 2
|
5,898.9 psi
|
Compressive strength of cylinder 3
|
5,895.2 psi
|
Type of fracture pattern of cylinder 2
|
2
|
Type of fracture pattern of cylinder 3
|
2
|
Comment on any defect in either specimen or caps (Max 250 Characters)
|
no data
|
Correction factor for cylinder 1
|
1.00
|
Correction factor for cylinder 2
|
1.00
|
Correction factor for cylinder 3
|
1.00
|
Age of specimen
|
56 days
|
Age of specimen in hours
|
no data0 hours
|