Sample Record for 2020-09-24-12
Note: Fields with no data or with a value of "Unknown" will not be displayed on the print out.
Project Information
Project ID: 214784 DEA: 023H8104 EFIS: 0218000036
QA Service Level: 1
DIST-CO-RTE-PM: 02-LAS,PLU-36,70,89,395-VAR
Work Description: PAINT BRIDGE STEEL, SEAL AND OVERLAY DECKS AND REPLACE BEARINGS.
Location Description: LASSEN AND PLUMAS COUNTIES AT VARIOUS LOCATIONS
Contractor Name: Q & D CONSTRUCTION, INC
Contractor Address: 1050 S 21st STREET, SPARKS, NV 89431
Resident Engineer: John Yolton Structure Rep.: Jeff Rothgery
Sample Information
DIME Sample ID: 2020-09-24-12
TL Number from the TL Form:
Sample Submitted By Organization: CT HQ - Sacramento Structural Materials Testing Laboratory
Sample Organization Contact: (916) 227-7253
Type of Sample: Quality Assurance
Type of Material: SMTL TM1 - Elastomeric Bearing Pad
Sample Taken Date: 09/24/2020
Date that the sample was received by the laboratory/organization performing the testing: 09/28/2020
The quantity of what the sample constitutes: 17
A brief description of the sample: Bearing Pad
From where was the sample collected: Manufacturer
Laboratory sample identification:
Structure unique identifier:
Structure name:
The fabricator/manufacturer/facility name: Scougal Rubber
Material Information
Mfg. Lot Number(s): 19002-1
Material/Compound/Elastomer ID: NA
Samples Representing: 1
Description (size): 2.3" x 8" x 8"
Comments:
Description (Number of Shims): 4
Type of Bearing Pad: Steel
Description (Thickness of Shims): 14 gage
Manufacturer(s): Scougal Rubber
Batch Number: NA
Test Results
Test 1 of 5
DIME Test ID: 2020-09-24-12-1
Test Method: ASTM D2240-05re10: Standard Test Method for Rubber Property - Durometer Hardness
Verified Date: 10/01/2020
Date Tested: 09/30/2020
Submitted By Organization: CT HQ - Sacramento Structural Materials Testing Laboratory
Organization Address: 5900 Folsom Boulevard,
Organization City: Sacramento
Organization State: CA
Organization Zipcode: 95819
Organization Email: paul.lukkarila@dot.ca.gov
Organization Phone: 916-227-7257
General Comments for this Test:
Test Result Compliance:
Additional Comments When Verified:
Temperature
|
72 f
|
Humidity
|
50 %
|
Reading #1
|
53
|
Reading #2
|
53
|
Reading #3
|
54
|
Reading #4
|
54
|
Reading #5
|
53
|
Mean
|
53.4
|
Test 2 of 5
DIME Test ID: 2020-09-24-12-2
Test Method: ASTM D412-06a-re13: Standard Test Methods for Vulcanized Rubber and Thermoplastic Elastomers-Tension
Verified Date: 10/01/2020
Date Tested: 09/30/2020
Submitted By Organization: CT HQ - Sacramento Structural Materials Testing Laboratory
Organization Address: 5900 Folsom Boulevard,
Organization City: Sacramento
Organization State: CA
Organization Zipcode: 95819
Organization Email: paul.lukkarila@dot.ca.gov
Organization Phone: 916-227-7257
General Comments for this Test:
Test Result Compliance:
Additional Comments When Verified:
Number of specimens tested
|
5
|
Unit of the Ultimate Tensile Values
|
lbf per sqr in
|
UTM
|
2kip
|
Humidity
|
50.00 %
|
Temperature
|
72 F
|
Sample 1 Median Thickness
|
0.084
|
Sample 1 Thickness all Within 0.003 inch?
|
Yes
|
Sample 1 Ultimate Tensile
|
2116.79 lbf/in^2
|
Sample 1 Elongation (350% Min)
|
Pass
|
Sample 2 Median Thickness
|
0.083
|
Sample 2 Thickness all Within 0.003 inch?
|
Yes
|
Sample 2 Ultimate Tensile
|
2211.83 lbf/in^2
|
Sample 2 Elongation (350% Min)
|
Pass
|
Sample 3 Median Thickness
|
0.087
|
Sample 3 Thickness all Within 0.003 inch?
|
Yes
|
Sample 3 Ultimate Tensile
|
2140.03 lbf/in^2
|
Sample 3 Elongation (350% Min)
|
Pass
|
Sample 4 Median Thickness
|
0.082
|
Sample 4 Thickness all Within 0.003 inch?
|
Yes
|
Sample 4 Ultimate Tensile
|
2169.23 lbf/in^2
|
Sample 4 Elongation (350% Min)
|
Pass
|
Sample 5 Median Thickness
|
0.087
|
Sample 5 Thickness all Within 0.003 inch?
|
Yes
|
Sample 5 Ultimate Tensile
|
2015.11 lbf/in^2
|
Sample 5 Elongation (350% Min)
|
Pass
|
Median of the Ultimate Tensile Values
|
2140 lbf/in^2
|
Test 3 of 5
DIME Test ID: 2020-09-24-12-3
Test Method: ASTM D624-00-re12: Standard Test Method for Tear Strength of Conventional Vulcanized Rubber and Thermoplastic Elastomers
Verified Date: 10/01/2020
Date Tested: 09/30/2020
Submitted By Organization: CT HQ - Sacramento Structural Materials Testing Laboratory
Organization Address: 5900 Folsom Boulevard,
Organization City: Sacramento
Organization State: CA
Organization Zipcode: 95819
Organization Email: paul.lukkarila@dot.ca.gov
Organization Phone: 916-227-7257
General Comments for this Test:
Test Result Compliance:
Additional Comments When Verified:
Number of specimens tested
|
3
|
UTM
|
2kip
|
Humidity
|
50.00 %
|
Temperature
|
72 F
|
Sample 1 Median Thickness
|
0.079
|
Sample 1 Tear Strength
|
237.3
|
Sample 2 Median Thickness
|
0.081
|
Sample 2 Tear Strength
|
233
|
Sample 3 Median Thickness
|
0.082
|
Sample 3 Tear Strength
|
230
|
Median of the Tear Strength Values
|
233 lb/in
|
Test 4 of 5
DIME Test ID: 2020-09-24-12-4
Test Method: ASTM D412-06a-re13: Standard Test Methods for Vulcanized Rubber and Thermoplastic Elastomers-Tension
Verified Date: 10/01/2020
Date Tested: 09/30/2020
Submitted By Organization: CT HQ - Sacramento Structural Materials Testing Laboratory
Organization Address: 5900 Folsom Boulevard,
Organization City: Sacramento
Organization State: CA
Organization Zipcode: 95819
Organization Email: paul.lukkarila@dot.ca.gov
Organization Phone: 916-227-7257
General Comments for this Test:
Test Result Compliance:
Additional Comments When Verified:
Number of specimens tested
|
5
|
Unit of the Ultimate Tensile Values
|
lbf per sqr in
|
UTM
|
2kip
|
Humidity
|
50.00 %
|
Temperature
|
72 F
|
Sample 1 Median Thickness
|
0.08
|
Sample 1 Thickness all Within 0.003 inch?
|
Yes
|
Sample 1 Ultimate Tensile
|
2303.01 lbf/in^2
|
Sample 1 Elongation (350% Min)
|
Pass
|
Sample 2 Median Thickness
|
0.08
|
Sample 2 Thickness all Within 0.003 inch?
|
Yes
|
Sample 2 Ultimate Tensile
|
1873.1 lbf/in^2
|
Sample 2 Elongation (350% Min)
|
Pass
|
Sample 3 Median Thickness
|
0.079
|
Sample 3 Thickness all Within 0.003 inch?
|
Yes
|
Sample 3 Ultimate Tensile
|
2262.28 lbf/in^2
|
Sample 3 Elongation (350% Min)
|
Pass
|
Sample 4 Median Thickness
|
0.078
|
Sample 4 Thickness all Within 0.003 inch?
|
Yes
|
Sample 4 Ultimate Tensile
|
2334.44 lbf/in^2
|
Sample 4 Elongation (350% Min)
|
Pass
|
Sample 5 Median Thickness
|
0.081
|
Sample 5 Thickness all Within 0.003 inch?
|
Yes
|
Sample 5 Ultimate Tensile
|
1951.21 lbf/in^2
|
Sample 5 Elongation (350% Min)
|
Pass
|
Median of the Ultimate Tensile Values
|
2262.3 lbf/in^2
|
Test 5 of 5
DIME Test ID: 2020-09-24-12-5
Test Method: SMTL BILST-06: (Neoprene Verification) Bilstein Test
Verified Date: 09/30/2020
Date Tested: 09/30/2020
Submitted By Organization: CT HQ - Sacramento Chemistry Laboratory
Organization Address: 5900 Folsom Boulevard,
Organization City: Sacramento
Organization State: CA
Organization Zipcode: 95819
Organization Email: sanchita.dey@dot.ca.gov
Organization Phone: (916) 227-7912
General Comments for this Test:
Test Result Compliance: complies
Additional Comments When Verified: