Unit system used?
|
US Units
|
Number of specimens
|
6
|
Test performed
|
With no density determined
|
Capped in accordance with?
|
ASTM C617/CTM521
|
Average diameter of cylinder 1
|
6.02 in
|
Average diameter of cylinder 2
|
6.00 in
|
Average diameter of cylinder 3
|
6.00 in
|
Average diameter of cylinder 4
|
6.01 in
|
Average diameter of cylinder 5
|
6.01 in
|
Average diameter of cylinder 6
|
6.01 in
|
Cross sectional area of cylinder 1
|
28.46 in^2
|
Cross sectional area of cylinder 2
|
28.27 in^2
|
Cross sectional area of cylinder 3
|
28.27 in^2
|
Cross sectional area of cylinder 4
|
28.37 in^2
|
Cross sectional area of cylinder 5
|
28.37 in^2
|
Cross sectional area of cylinder 6
|
28.37 in^2
|
Compressive strength (to nearest 10 psi)
|
2490 psi
|
Maximum load on cylinder 1
|
50320 lb
|
Maximum load on cylinder 2
|
90180 lb
|
Maximum load on cylinder 3
|
90300 lb
|
Maximum load on cylinder 4
|
89015 lb
|
Maximum load on cylinder 5
|
52245 lb
|
Maximum load on cylinder 6
|
51935 lb
|
Compressive strength of cylinder 1
|
1768.1 psi
|
Type of fracture pattern of cylinder 1
|
2
|
Compressive strength of cylinder 2
|
3190.0 psi
|
Compressive strength of cylinder 3
|
3194.2 psi
|
Compressive strength of cylinder 4
|
3137.6 psi
|
Compressive strength of cylinder 5
|
1841.6 psi
|
Compressive strength of cylinder 6
|
1830.6 psi
|
Type of fracture pattern of cylinder 2
|
2
|
Type of fracture pattern of cylinder 3
|
1
|
Type of fracture pattern of cylinder 4
|
2
|
Type of fracture pattern of cylinder 5
|
1
|
Type of fracture pattern of cylinder 6
|
3
|
Comment on any defect in either specimen or caps (Max 250 Characters)
|
no data
|
Correction factor for cylinder 1
|
1
|
Correction factor for cylinder 2
|
1
|
Correction factor for cylinder 3
|
1
|
Correction factor for cylinder 4
|
1
|
Correction factor for cylinder 5
|
1
|
Correction factor for cylinder 6
|
1
|
Age of specimen
|
7 days
|
Age of specimen in hours
|
no data
|