Print Report | Back to Sample Detail

Sample Record for 2025-09-03-74

Note: Fields with no data or with a value of "Unknown" will not be displayed on the print out.

Project Information

Project ID: 1000272 DEA: 100V4804 EFIS: 1013000264 QA Service Level: 1
DIST-CO-RTE-PM: 10-CAL-26-21.8/30.3
Work Description: SLOPE STABILIZATION AND CONSTRUCT RETAINING WALL.
Location Description: CALAVERAS COUNTY NEAR MOKELUMNE HILL AT VARIOUS LOCATIONS FROM 3.6 MILES EAST OF ROUTE 49 TO 0.9 MILE WEST OF WOODHOUSE MINE ROAD
Contractor Name: VIKING CONSTRUCTION COMPANY, INC.
Contractor Address: Unknown
Resident Engineer: Jonathan Ngai Structure Rep.: Conor Hennessy

Sample Information

DIME Sample ID: 2025-09-03-74
TL Number from the TL Form: 115268
Sample Submitted By Organization: CT SC - 3665 - Shingle Springs
Sample Organization Contact: (530) 821-8266
Type of Sample: Quality Assurance
Type of Material: Concrete
Sample Taken Date: 09/03/2025
Date that the sample was received by the laboratory/organization performing the testing: 09/04/2025
The quantity of what the sample constitutes: 12 Cylinders
A brief description of the sample: 4x8 concrete cylinders
From where was the sample collected: Job Site
Laboratory sample identification:
Structure unique identifier:
Structure name: Wall 2
The fabricator/manufacturer/facility name: 711 materials

Material Information

The concrete mix design number: 800811A
The truck number from where the sample was collected:
The batch plant ticket number from where the sample was collected: Unknown
Concrete batch plant:
The fabricator/manufacturer designation for the sample:
A detailed description of where the material sample was collected: Chute
Where the material sample would have been placed if not sampled:
From Lot No.:
Bag Lot No.:

Test Results

Test 1 of 4

DIME Test ID: 2025-09-03-74-1
Test Method: ASTM C39-17a: Standard Test Method for Compressive Strength of Cylindrical Concrete Specimens
Verified Date: 10/03/2025
Date Tested: 09/17/2025
Submitted By Organization: CT SC - 3665 - Shingle Springs
Organization Address: 3976 Durock Road, Suite 102,
Organization City: Shingle Springs
Organization State: CA
Organization Zipcode: 95686
Organization Email: brandon.miller@dot.ca.gov
Organization Phone: (530) 821-8266
General Comments for this Test: Tested by Stockton District Lab
Test Result Compliance:
Additional Comments When Verified:
Unit system used? US Units
Number of specimens 3
Test performed With no density determined
Capped in accordance with? ASTM C1231 - Unbonded Elastomeric Pad Cap
Average diameter of cylinder 1 4.00 in
Average diameter of cylinder 2 4.00 in
Average diameter of cylinder 3 4.00 in
Cross sectional area of cylinder 1 12.57 in^2
Cross sectional area of cylinder 2 12.57 in^2
Cross sectional area of cylinder 3 12.57 in^2
Compressive strength (to nearest 10 psi) 4360 psi
Maximum load on cylinder 1 59340 lb
Maximum load on cylinder 2 54270 lb
Maximum load on cylinder 3 50740 lb
Compressive strength of cylinder 1 4720.8 psi
Type of fracture pattern of cylinder 1 3
Compressive strength of cylinder 2 4317.4 psi
Compressive strength of cylinder 3 4036.6 psi
Type of fracture pattern of cylinder 2 3
Type of fracture pattern of cylinder 3 2
Comment on any defect in either specimen or caps (Max 250 Characters) no data
Correction factor for cylinder 1 1
Correction factor for cylinder 2 1
Correction factor for cylinder 3 1
Age of specimen 14 days
Age of specimen in hours no data

Test 2 of 4

DIME Test ID: 2025-09-03-74-2
Test Method: ASTM C39-17a: Standard Test Method for Compressive Strength of Cylindrical Concrete Specimens
Verified Date: 10/03/2025
Date Tested: 09/24/2025
Submitted By Organization: CT SC - 3665 - Shingle Springs
Organization Address: 3976 Durock Road, Suite 102,
Organization City: Shingle Springs
Organization State: CA
Organization Zipcode: 95686
Organization Email: brandon.miller@dot.ca.gov
Organization Phone: (530) 821-8266
General Comments for this Test: Tested by Stockton District Lab
Test Result Compliance:
Additional Comments When Verified:
Unit system used? US Units
Number of specimens 3
Test performed With no density determined
Capped in accordance with? ASTM C1231 - Unbonded Elastomeric Pad Cap
Average diameter of cylinder 1 4.01 in
Average diameter of cylinder 2 4.02 in
Average diameter of cylinder 3 4.01 in
Cross sectional area of cylinder 1 12.63 in^2
Cross sectional area of cylinder 2 12.69 in^2
Cross sectional area of cylinder 3 12.63 in^2
Compressive strength (to nearest 10 psi) 4930 psi
Maximum load on cylinder 1 60020 lb
Maximum load on cylinder 2 60910 lb
Maximum load on cylinder 3 66320 lb
Compressive strength of cylinder 1 4752.2 psi
Type of fracture pattern of cylinder 1 2
Compressive strength of cylinder 2 4799.8 psi
Compressive strength of cylinder 3 5251 psi
Type of fracture pattern of cylinder 2 2
Type of fracture pattern of cylinder 3 3
Comment on any defect in either specimen or caps (Max 250 Characters) no data
Correction factor for cylinder 1 1
Correction factor for cylinder 2 1
Correction factor for cylinder 3 1
Age of specimen 21 days
Age of specimen in hours no data

Test 3 of 4

DIME Test ID: 2025-09-03-74-3
Test Method: ASTM C39-17a: Standard Test Method for Compressive Strength of Cylindrical Concrete Specimens
Verified Date: 10/03/2025
Date Tested: 10/01/2025
Submitted By Organization: CT SC - 3665 - Shingle Springs
Organization Address: 3976 Durock Road, Suite 102,
Organization City: Shingle Springs
Organization State: CA
Organization Zipcode: 95686
Organization Email: brandon.miller@dot.ca.gov
Organization Phone: (530) 821-8266
General Comments for this Test: Tested by D10 Stockton Lab
Test Result Compliance:
Additional Comments When Verified:
Unit system used? US Units
Number of specimens 3
Test performed With no density determined
Capped in accordance with? ASTM C1231 - Unbonded Elastomeric Pad Cap
Average diameter of cylinder 1 4.00 in
Average diameter of cylinder 2 4.01 in
Average diameter of cylinder 3 4.01 in
Cross sectional area of cylinder 1 12.57 in^2
Cross sectional area of cylinder 2 12.63 in^2
Cross sectional area of cylinder 3 12.63 in^2
Compressive strength (to nearest 10 psi) 5350 psi
Maximum load on cylinder 1 67140 lb
Maximum load on cylinder 2 65400 lb
Maximum load on cylinder 3 69670 lb
Compressive strength of cylinder 1 5341.3 psi
Type of fracture pattern of cylinder 1 2
Compressive strength of cylinder 2 5178.1 psi
Compressive strength of cylinder 3 5516.2 psi
Type of fracture pattern of cylinder 2 3
Type of fracture pattern of cylinder 3 2
Comment on any defect in either specimen or caps (Max 250 Characters) no data
Correction factor for cylinder 1 1
Correction factor for cylinder 2 1
Correction factor for cylinder 3 1
Age of specimen 28 days
Age of specimen in hours no data

Test 4 of 4

DIME Test ID: 2025-09-03-74-4
Test Method: ASTM C39-17a: Standard Test Method for Compressive Strength of Cylindrical Concrete Specimens
Verified Date: 10/03/2025
Date Tested: 10/01/2025
Submitted By Organization: CT SC - 3665 - Shingle Springs
Organization Address: 3976 Durock Road, Suite 102,
Organization City: Shingle Springs
Organization State: CA
Organization Zipcode: 95686
Organization Email: brandon.miller@dot.ca.gov
Organization Phone: (530) 821-8266
General Comments for this Test: Tested by D10 Stockton Lab
Test Result Compliance:
Additional Comments When Verified:
Unit system used? US Units
Number of specimens 3
Test performed With no density determined
Capped in accordance with? ASTM C1231 - Unbonded Elastomeric Pad Cap
Average diameter of cylinder 1 4.00 in
Average diameter of cylinder 2 3.98 in
Average diameter of cylinder 3 4.00 in
Cross sectional area of cylinder 1 12.57 in^2
Cross sectional area of cylinder 2 12.44 in^2
Cross sectional area of cylinder 3 12.57 in^2
Compressive strength (to nearest 10 psi) 5530 psi
Maximum load on cylinder 1 64780 lb
Maximum load on cylinder 2 71720 lb
Maximum load on cylinder 3 71160 lb
Compressive strength of cylinder 1 5153.5 psi
Type of fracture pattern of cylinder 1 3
Compressive strength of cylinder 2 5765.3 psi
Compressive strength of cylinder 3 5661.1 psi
Type of fracture pattern of cylinder 2 3
Type of fracture pattern of cylinder 3 2
Comment on any defect in either specimen or caps (Max 250 Characters) no data
Correction factor for cylinder 1 1
Correction factor for cylinder 2 1
Correction factor for cylinder 3 1
Age of specimen 28 days
Age of specimen in hours no data